Overview
Section 1 - Mix
User
harare
Type1
Blended Cement
Type2
General Use
Mix ID
183
Materials
Material
Weight g (%)
Material Family
Commercial Name
Price
True Density
Bulk Density (g/cc)

Aurubis slag 2700 cm2/g
40 (8.89 %)
Industrial Slag / Glass

CEM I 52.5R
44.4 (9.87 %)
Portland Cement

Limestone powder
15.6 (3.47 %)
Mineral

Water
50 (11.11 %)
Water

Standard sand
300 (66.67 %)
Fine Aggregate

Placing & Curing
Shaping
De-Airing
Curing conditions
Duration (Mins)
Conditions after curing
Duration (Mins)

Casting
Jolting
20-22°C & 60-70% Humidity

Open

Fresh Properties
Standard (Mortar)
Standard (Concrete)
Value
Standard Deviation

-
-
187.5
0.71

Hardened Properties
Standard (Mortar)
Standard (Concrete)
Value
Standard Deviation

-
-
10.2
0.34

-
-
20.9
1.06

-
-
38.9
3.77