Overview
Section 1 - Mix
User
harare
Type1
Blended Cement
Type2
General Use
Mix ID
194
Materials
Material
Weight g (%)
Material Family
Commercial Name
Price
True Density
Bulk Density (g/cc)

Aurubis slag 4400 cm2/g
30 (0.0667 %)
Industrial Slag / Glass

CEM I 52.5R
45.2 (0.1004 %)
Portland Cement

Limestone powder
24.8 (0.0551 %)
Mineral

Water
50 (0.1111 %)
Water

Standard sand
300 (0.6667 %)
Fine Aggregate

Placing & Curing
Shaping
De-Airing
Curing conditions
Duration (Mins)
Conditions after curing
Duration (Mins)

Casting
Jolting
20-22°C & 60-70% Humidity

Open

Fresh Properties
Standard (Mortar)
Standard (Concrete)
Value
Standard Deviation

-
-
192.5
0.71

Hardened Properties
Standard (Mortar)
Standard (Concrete)
Value
Standard Deviation

-
-
12.5
0.08

-
-
20.7
0.45

-
-
35.9
2.45